Designing and drawing weldments
In a weldment, the process fights the drawing. Every weld shrinks as it cools and pulls the frame out of square, so holes drilled before welding wander and faces that were flat go wavy. A good weldment drawing plans for that: it keeps welds small and balanced, machines the accurate features after welding, and defines every joint with a weld symbol or a weld note instead of leaving the welder to guess. This guide covers the design rules, how weld symbols work, where datums go, and the tolerances fabrication shops hold.
Design rules for weldments
Welding melts metal along a joint, and the joint shrinks as it cools. That pulls the parts out of position. Most weldment rules are about controlling that distortion, giving the welder access, and deciding what gets machined after welding.
| Rule | Typical value | Why |
|---|---|---|
| Use standard shapes | plate, tube, angle, channel and beam from stock sizes | Standard stock is cheap, available, and easy to cut and fit. |
| Fewer, smaller welds | weld only the joints the function needs, at the size it needs | Every weld adds heat, distortion and cost. An oversized fillet doesn't add useful strength; it adds distortion. |
| Minimum fillet size by thickness | 3 mm for parts up to 6 mm thick, 5 mm up to 12 mm, 6 mm up to 20 mm, 8 mm above (AWS D1.1 minimums for steel, set by the thicker part; the weld needn't exceed the thinner part) | Too small a fillet on thick plate cools too fast and can crack. These are minimums, not strength calculations: size load-bearing welds by calculation. |
| Balance the welds | weld symmetrically about the part's neutral axis, or in a sequence | Welds on one side only bow the part. |
| Access | leave room for the torch or gun at the right angle, and for the welder to see the joint | A joint the welder can't reach can't be welded well. |
| Machine after welding | anything that must be accurate: mounting faces, bearing bores, dowel holes | Welding moves pre-machined features. Machining after welding puts them where they belong. |
| Crop corners on gussets | cut the inside corner of gussets and stiffeners | Lets the welds pass, and on galvanized parts lets zinc, air and cleaning acid flow through instead of collecting in pockets. |
| Vent and drain hollow parts for galvanizing | a vent at the highest and a drain at the lowest point of every closed section, as it hangs in the bath; sized to the section per ASTM A385, for example about 13 mm pairs on 50 mm square tube, 25 mm on 100 mm and 40 mm on 150 mm, or one opening of about 25 to 30% of the section area | Sealed sections can burst in the zinc bath, and trapped zinc or acid ruins the coating. Your galvanizer will confirm the sizes. |
More calculators in the Toolbox
What the drawing must say
One drawing for the whole weldment. The weldment drawing defines the finished, welded part. One fabricator owns it, because overall dimensions can only be held by whoever welds the whole thing. Don't detail the members on separate drawings for different shops. The drawing has:
- assembly views, with a balloon for each member;
- a parts list (cut list): item, quantity, description, stock size, length and material;
- weld symbols on every joint that is welded;
- dimensions and tolerances, with post-weld machining clearly marked.
Weld symbols follow AWS A2.4, not Y14.5. GD&T still controls the dimensions. ISO 2553 draws the arrow side differently, with a dashed identification line, so say which standard the drawing follows and never mix the two. Every joint gets either a complete weld symbol, or a general weld note with exceptions, such as UNLESS OTHERWISE SPECIFIED, ALL JOINTS 5 FILLET ALL AROUND. Never leave joints undefined, and never assume every contact is welded. Every fillet has a size. For a groove weld with no depth given, the symbol means complete joint penetration, so say so when that's what you want.
Datums. If anything is machined after welding, put the datums on the machined features: a machined mounting face as A, and machined holes as B and C. If nothing is machined, A is the base member's mounting face. On large frames that distort, use datum targets, and a restraint note if the frame is clamped for inspection.
Tolerances. Fabrication shops work from a size-banded table, not one tolerance for every size. A 25 mm dimension and a 3 m dimension can't share the same ±. Print the table on the drawing (values below), or cite the standard and class in a note, for example ISO 13920-BF, where B is the linear and angular class and F the straightness and flatness class. Holes drilled before welding get a loose position, because welding moves them. Anything tighter is machined after welding and toleranced like a machined part. Squareness of a frame can be a perpendicularity or profile tolerance, or on a large frame a note that the diagonals are equal within a value.
Notes a weldment needs:
- Welding code: AWS D1.1 for structural steel, D1.3 for sheet steel, D1.2 for aluminum, D1.6 for stainless.
- Welder or procedure qualification, if required.
- Inspection: always stated. Either visual inspection per the code with no other NDE, or the method and acceptance criteria.
MACHINE AFTER WELDINGon the features that are, and the stress relief cycle if machining or flatness depends on it. Give a specification or the temperature and time (for carbon steel typically about 600 °C, held about an hour per 25 mm of thickness; confirm it against the material specification). A bare "stress relieve" leaves the cycle to guesswork. Stress relief doesn't remove distortion; design, weld sequence and heat input control that.- Spatter removal, and grinding flush where needed.
- Coating: for hot-dip galvanizing, galvanize after fabrication per ASTM A123, with venting and draining per ASTM A385. Mask or retap threads.
- The delivered condition: as-welded, stress-relieved, machined or coated.
Typical tolerances
| Tier | Typical value | What it takes | Cost |
|---|---|---|---|
| As welded | ISO 13920 class B: ±1 mm up to 30 mm, ±2 to 400 mm, ±3 to 1000 mm, ±4 to 2000 mm. Angles ±45′ up to 400 mm, ±30′ to 1000 mm, ±20′ beyond (by the shorter leg). Holes drilled before welding: a loose position, typically about Ø3. | Good fit-up and a sensible weld sequence | Standard |
| Fixtured and straightened | about ISO 13920 class A: ±1 mm up to 400 mm, ±2 to 1000 mm, ±3 to 2000 mm; angles ±20′, ±15′, ±10′ | Welding fixtures, tack-and-check, straightening, sometimes stress relief | Fixture cost, plus labor per part |
| Machined after welding | machining capability (see the CNC guide), to machined datums | A machine large enough for the whole weldment, usually stress relief first | An extra operation and setup; often the cheapest way to get accuracy on a large part |
Worked example: a machine base frame (illustrative)
A base frame is welded from 80 × 80 × 5 mm square steel tube, with a 20 mm top plate that's machined after welding, and then galvanized. The diagram is an illustration, not a drawing from the app.
| On the drawing | What it says | Why |
|---|---|---|
| Parts list: tube (cut lengths), top plate, foot plates, gussets | Every member, its stock size and length | The fabricator buys and cuts from it. |
Weld symbols: 5 fillet all around at each tube joint; 6 fillet on the top plate, intermittent 50-150 on the long sides | Every welded joint, with its size, length and pitch | Nothing is assumed. The intermittent welds limit heat and distortion on the plate. |
MACHINE AFTER WELDING: top face flat 0.1, datum A; two dowel holes B and C positioned to A | The mounting surface and locating holes are machined last | The machine mounted on top needs a flat, accurate face that welding would distort. |
| Stress relief note with temperature and time, before machining | The weldment is relaxed before the precision features are cut | Otherwise the machined face moves when residual stress is released. |
| Anchor holes in the feet, drilled before welding, position Ø3 | Holes that only need to clear anchor bolts | No reason to machine them after welding. |
| Tolerance table on the sheet (±1 / ±2 / ±3 / ±4 by size) | Everything not machined is held to fabrication tolerances | That's what welding holds. |
| Galvanize per ASTM A123 after fabrication; vent and drain holes at each tube's ends (about Ø20 mm pairs for this tube); machined face and dowel holes masked | The coating and how to get it on safely | Sealed tubes can burst in the zinc bath, and zinc on the machined face would ruin its flatness. |
| Visual inspection per AWS D1.1; no other NDE | The acceptance level is stated | "Good welds" isn't a requirement. |
Common mistakes
- "Weld all joints", or no weld symbols. The fabricator has to guess which joints, what size and how long. Give each joint a symbol, or a default weld note with listed exceptions.
- Machining tolerances on as-welded features. A hole drilled before welding won't stay within ±0.1 after welding. Put the tight features on machined surfaces, after welding.
- Closed sections without vents. For galvanizing they're a safety hazard, and for painting they trap moisture. Add vent and drain holes and show them.
- Members detailed for different shops. No one can then hold the overall dimensions. One fabricator, one weldment drawing.
- "Stress relieve" with no cycle, and no inspection stated. Give the specification or the temperature and time, and name the NDE method and acceptance, even if it's visual only.
Questions
How do you read a weld symbol?
The arrow points to the joint. The symbol below the reference line applies to the arrow side of the joint, and the symbol above it to the other side. The size goes to the left of the weld symbol and the length and pitch to the right. Where the arrow meets the reference line, a circle means weld all around and a flag means a field weld. The tail carries a process or specification reference. Weld symbols follow AWS A2.4; ISO 2553 places the arrow-side symbol differently.
Where should datums go on a weldment?
On the features machined after welding, if there are any: a machined mounting face as datum A and machined holes as B and C. If nothing is machined, use the base member's mounting face, and datum targets on large frames that distort.
What tolerance can a weldment hold?
Fabrication tolerances grow with size, so shops work from a size-banded table rather than one ± for every dimension. ISO 13920 class B, a common default, allows ±1 mm up to 30 mm, ±2 mm up to 400 mm, ±3 mm up to 1000 mm and ±4 mm up to 2000 mm. Anything that has to be tighter is machined after welding and toleranced like a machined part.
Should holes be drilled before or after welding?
Holes that only need to be roughly placed can go in before welding, with a loose position tolerance. Holes that locate other parts, such as dowel and bearing holes, are machined after welding, because welding moves them.
What notes does a weldment drawing need?
The welding code (for example AWS D1.1 for structural steel), the inspection requirement, which features are machined after welding, any stress relief cycle, the coating, and the delivered condition.
Sources
- AWS A2.4, Standard Symbols for Welding, Brazing, and Nondestructive Examination, and ISO 2553, Welding and allied processes: symbolic representation on drawings
- AWS D1.1, Structural Welding Code: Steel (minimum fillet weld sizes, via TWI below)
- TWI, How do you determine the minimum size of a fillet weld?
- ISO 13920:2023, Welding: general tolerances for welded constructions (classes A to D and E to H; public preview)
- American Galvanizers Association, Required vent and drain holes for hollow structural sections and Rectangular and square HSS venting alternatives (ASTM A385 sizes)
- ASTM A123 (hot-dip galvanizing) and ASTM A385 (practice for providing high-quality zinc coatings)
- Metallurgy for Machinists, Stress relieving
- ASME Y14.5-2018, Dimensioning and Tolerancing