Designing and drawing parts for 3D printing
3D printing removes many machining limits, but it adds its own. A wall that prints fine on a resin printer can be too thin for powder nylon. A hole drawn at nominal size comes out small. A tolerance that is easy in the plane of the layers is about twice as hard to hold in the build direction. And a drawing that treats a printed part like a machined one ends in scrap or an argument. This guide covers the design rules for the common processes (FDM, SLA, SLS, MJF and metal powder bed fusion), the tolerances each holds as built, and what the drawing has to say.
Design rules for 3D printed parts
A printed part is built in layers, so its accuracy, strength and surface depend on the direction it's built in. Some processes need supports under overhangs, and the supports leave marks. Powder and resin processes can trap material inside hollow parts. Most rules come from those three facts.
Reliable design values (the hard minimum the printer can just manage is smaller; design to these):
| Rule | FDM | SLA (resin) | SLS / MJF (nylon powder) | Metal (laser powder bed fusion) |
|---|---|---|---|---|
| Wall thickness | 1.2 mm (0.8 minimum, two perimeters of a 0.4 nozzle) | 0.6 mm unsupported, 0.4 mm supported (some newer printers 0.2) | 1.0 mm (about 0.8 minimum for SLS, 0.5 for MJF) | 1.0 mm (0.5 in titanium, cobalt chrome and stainless) |
| Overhang without support | 45° or steeper from horizontal; bridges up to about 5 mm | Usually printed on supports; short overhangs (about 1 to 5 mm, by printer) can go without | No supports needed: the powder holds the part | About 45° or steeper is the usual limit; any overhang over about 0.8 mm needs support |
| Small holes | Print undersized; drill or ream if the size matters | Print slightly undersized; drill or ream for fits | 1.5 mm reliable (1.0 minimum); smaller holes can fuse shut | Under about 1 mm may close; machine fits after the build |
| Clearance between parts | 0.2 to 0.4 mm | 0.5 mm for moving parts, 0.2 mm for parts assembled afterwards | 0.4 to 0.6 mm for parts assembled afterwards; 0.7 to 1.0 mm for parts printed already assembled | Machine mating features |
| Hollow parts | — | Drain holes so trapped resin can escape | At least two escape holes, about 3.5 mm or larger | Powder escape holes, plus a way to check the inside is clear |
| Threads | Heat-set or press-in inserts | Inserts | Inserts | Machined after the build |
Two rules apply to every process:
- Build direction matters. Tolerances in the build (Z) direction are roughly twice as loose as in the plane of the layers (XY). Shallow slopes show steps, and surfaces facing down are rougher. On metal parts they are also where supports attach. Decide the orientation before you set tolerances.
- Machine what has to be accurate. Bores, sealing faces, threads and datum faces that must be precise are machined or reamed after printing. The model then needs extra stock on those surfaces.
More calculators in the Toolbox
What the drawing must say
Standards. ASME Y14.8, the standard for castings, forgings and molded parts, does not cover additive parts. A printed part is drawn to ASME Y14.5 and Y14.100 like any other part. ASME Y14.46 (product definition for additive manufacturing) applies when the customer works to it. The ISO/ASTM 52911 series gives design guidance for powder bed processes. It's a design aid, not a drawing standard.
Datums on what mates. Use the features that locate the part in assembly, as for any part. If those surfaces are machined after printing, the machined surfaces become the datums for the accurate features, and the as-built surfaces are toleranced to them.
A general profile at what the process holds. One note controls all as-built surfaces with a profile to the datums. Typical values are about 0.6 mm and up for polymer powder processes and about 0.3 mm for small metal powder bed parts, growing with size. Check them against your vendor's published tolerances. Tighter callouts go only on machined features, at machining capability.
Notes a printed part needs:
- Material and process, spelled out: for example
Ti-6Al-4V PER ASTM F2924, LASER POWDER BED FUSION, orPA12, POWDER BED FUSION. Name a trade-named process only if the customer requires it. - Build orientation, shown on the pictorial view, when it affects the requirements.
- Post-processing: stress relief, hot isostatic pressing (HIP) or heat treatment, each with its specification, and bead blasting or other finishing.
- Two surface texture defaults: one for as-built surfaces and one for machined surfaces. Down-facing surfaces may need their own value.
- Support marks: surfaces where supports aren't allowed, or how much witness may remain.
- Internal channels and lattices: that powder must be removed, and how it's checked (CT scanning if it's critical).
- Inserts by part number and the maker's installation document.
- Inspection: any NDE, stated explicitly.
Typical tolerances
As built, before any machining. Vendors publish different figures for the same process, so treat these as typical and check your vendor's table:
| Process | Typical as-built tolerance |
|---|---|
| FDM | industrial machines about ±0.3 %, not tighter than ±0.3 mm; prototyping grades about ±0.5 %, not tighter than ±0.5 mm |
| SLA | industrial machines about ±0.05 mm plus 0.1 % of the length (about ±0.15 mm at 100 mm); desktop printers about ±0.2 to 0.3 % on larger parts |
| SLS (nylon) | about ±0.3 %, not tighter than ±0.3 mm (some services ±0.25 mm plus 0.1 %) |
| MJF (nylon) | about ±0.25 to ±0.4 mm in the layer plane up to 80 mm on reviewed production orders, about 1.7× that in the build direction; prototype grades much looser |
| Metal (laser powder bed) | about ±0.075 mm plus 0.1 % of the length in the layer plane, about twice that in the build direction |
| Tier | What it means | What it costs |
|---|---|---|
| General | The as-built values above, written as a general profile (about 0.6 mm and up for polymer powder, about 0.3 mm on small metal parts) | Nothing extra |
| Tight | Tighter as-built values on a few features, with the orientation chosen for them and test prints to dial in the size | Extra iterations, and often a worse orientation for other features |
| Very tight | Machined, drilled or reamed after printing, at machining capability (typically ±0.025 to 0.05 mm, see the CNC guide) | A machining operation and a fixture for an irregular part. The model must carry the extra stock. |
Worked example: a printed titanium bracket (illustrative)
A Ti-6Al-4V bracket is printed by laser powder bed fusion, then HIPed, then two features are machined. The diagram is an illustration, not a drawing from the app.
| On the drawing | What it says | Why |
|---|---|---|
| Datum A on the machined mounting face; datum B on the reamed bore | The datums are the surfaces that mate, and both are machined | As-built surfaces are too rough and too variable to locate from precisely. |
Bore Ø10.000-10.015 (10 H7), position to A | A fit, machined after printing | No printer holds an H7 fit as-built. |
| General profile 0.3 to A and B on as-built surfaces | Everything else stays as printed | That's what laser powder bed fusion holds. Nothing is machined that doesn't need to be. |
| Two texture defaults: as-built (for example Ra 12.5 µm, from the vendor's as-built data) and machined (Ra 1.6 on the bore and face) | Each kind of surface has its own requirement | One default would either reject every as-built surface or under-specify the machined ones. |
| Material note with the ASTM specification, process name and HIP specification | What the part is made of and how | Properties of printed metal depend on the process and post-processing, not just the alloy. |
| Build direction shown on the pictorial view; no supports on the bore face | The orientation the tolerances assume | Turning the part changes which faces are rough and which directions are accurate. |
Common mistakes
- One tolerance in every direction. The build direction is roughly twice as loose as the layer plane. Choose the orientation first, then set the tolerances.
- Tight tolerances on as-built surfaces. A fit, a seal or a thread is machined, reamed or given an insert. Asking the printer for ±0.02 just means scrap.
- No way out for powder or resin. Hollow parts and internal channels need escape holes, and a drawing note on how the inside is checked.
- Holes and threads drawn at nominal size. Small holes print undersized, and printed threads in plastic wear quickly. Plan to drill or ream the holes, and use inserts for threads.
- Overhangs without a support plan. Supports leave marks and cost removal time. Keep overhangs at 45° or steeper on processes that need supports, and say which surfaces must stay free of supports.
Questions
What is the minimum wall thickness for 3D printing?
It depends on the process. Reliable design values are about 1.2 mm for FDM, 0.4 to 0.6 mm for SLA, 1.0 mm for SLS and MJF nylon, and 1.0 mm for metal powder bed fusion (0.5 mm in titanium, cobalt chrome and stainless). Printers can go thinner, but those walls are fragile and inconsistent.
What tolerance can 3D printing hold?
As built on a part around 50 to 100 mm, roughly ±0.1 to 0.15 mm for industrial SLA, ±0.3 mm or ±0.3 % for SLS and FDM, ±0.25 to 0.4 mm for MJF in the layer plane, and ±0.1 to 0.2 mm for metal powder bed fusion. The build direction is looser than the layer plane, and vendors publish different tables, so check yours. Anything tighter is machined, drilled or reamed after printing.
Which is more accurate, FDM or SLS?
Industrial FDM and SLS land in a similar range, about ±0.3 % with a ±0.3 mm floor. SLS needs no supports and handles complex shapes better. SLA usually gives the finest detail and the smoothest surface of the common polymer processes, and is among the most accurate on small parts.
Does a 3D printed part need a drawing?
For prototypes, often not. For production, or any part with fits, threads, machined features or inspection requirements, yes. The model cannot say which surfaces are machined, what the build orientation is, which post-processing is required, or how the part is inspected.
Which standard covers drawings of 3D printed parts?
ASME Y14.5 for dimensioning and tolerancing, as for any part. ASME Y14.46 covers product definition for additive manufacturing when the customer works to it. ASME Y14.8 covers castings, forgings and molded parts, not additive.
Sources
- Protolabs, 3D printing service pages: FDM, SLA, SLS and DMLS (walls, tolerances)
- Protolabs, 7 mistakes to avoid when designing 3D printed parts (metal walls, holes, overhangs)
- Hubs (Protolabs Network) design guides: FDM, SLA, SLS and MJF
- HP, How to design a 3D print model (MJF walls and clearances)
- Formlabs, Form 4 design guide and Design specifications for Fuse 1
- Xometry, HP Multi Jet Fusion (MJF tolerances)
- ISO/ASTM 52911-1, -2 and -3, Additive manufacturing: design for powder bed fusion
- ASME Y14.5-2018, Dimensioning and Tolerancing, and ASME Y14.46, Product Definition for Additive Manufacturing