Guides

Designing and drawing sheet metal parts

Sheet metal fails on paper long before it fails in the shop. A hole drawn too close to a bend comes out oval. A ±0.05 across two bends cannot be held by bending alone. A thickness given as "14 GA" means one thing in steel and another in aluminum. This guide covers the design rules fabricators work to, how bends move material, the tolerances they can actually hold, and what a sheet metal drawing has to say.

Design rules for sheet metal

Sheet metal is cut flat (laser, punch or waterjet) and then bent on a press brake. Features in one flat are cut in a single setup and land accurately. Every bend adds error, and metal near a bend stretches. Most rules follow from that.

RuleTypical valueWhy
Inside bend radiusone radius for the whole part, about 1× the thickness (T), never below the minimum for the alloy and temperEach radius needs its own tooling. Too small a radius cracks the outside of the bend, especially in harder tempers.
Hole to bendkeep holes about 4T or more from a bend (some fabricators use 2.5T + R from the inside of the bend)Closer holes stretch into ovals when the flange is bent.
Hole to part edgeat least 1.6 mm for sheet up to about 0.9 mm thick; at least 3.2 mm for thicker sheetA thin bridge of material tears or bulges when punched.
Hole to holeweb ≥ TA thinner web distorts.
Hole diameter≥ TA punch smaller than the thickness breaks. A laser can go smaller, but the edge quality drops.
Flange length≥ 4TThe flange has to span the die opening to bend cleanly.
Bend reliefwidth at least T, depth at least the bend radius (R + T is common), where a bend ends at an edgeWithout relief the corner tears, or the material bulges.
Self-clinching hardwarecatalog hole size and edge distance, kept outside the bend radius, with the install side statedThe hardware needs flat, undisturbed material to clinch into.
Grain directionspecify it only for tight bends in harder alloysBending across the grain cracks less.
The flat blank where a bend ends at an edge, twice. Without a relief the corner at the end of the bend line tears or bulges. With a relief cut at least T wide and at least R deep it does not.
Bend relief: a small cut at the end of the bend line, at least T wide and at least the bend radius R deep.
A flat sheet metal blank with a bend line and two holes. The hole about 4T or more from the bend line stays round. The hole closer to the bend line stretches into an oval when the flange is formed.
Hole to bend: about 4T or more keeps the hole round.

Bend allowance and the K-factor

The flat blank is shorter than the outside dimensions of the formed part, because the metal stretches on the outside of each bend and compresses on the inside. Somewhere inside the thickness is a neutral line that keeps its length. The K-factor says where that line sits, as a fraction of the thickness from the inside surface: typically 0.3 to 0.5. For air bending it's about 0.33 to 0.44 when the radius is up to T, 0.40 to 0.48 from T to 3T, and about 0.5 above that, depending on the material (see the chart below).

The length of the neutral line through one bend, the bend allowance, is:

BA = (π / 180) × bend angle in degrees × (R + K × T)

The flat length is the straight lengths of the flanges, measured to the tangent points where each bend starts, plus one bend allowance per bend. The K-factor depends on the material, thickness, radius and the shop's tooling, so the shop sets it. The drawing gives the formed dimensions. A flat pattern, if you include one, is marked reference only.

A 90 degree bend in section. The inside radius R, the thickness T, the neutral line K times T from the inside surface, and the bend allowance BA, the length of the neutral line through the bend.
The neutral line keeps its length. The flat blank is the two straight flanges plus the bend allowance.

Bend allowance chart: typical starting K

Typical starting values for air bending, from one press brake maker's published chart (Durma). Aluminum and mild steel agree with other published figures; stainless has no second source. A test bend on your own tooling beats any table. In the key below, A is the bend angle (not the included angle) and R is the radius the part forms; in air bending that comes mostly from the die opening, not the punch.

BA = (π / 180) × A × (R + K × T), with A in degrees. For a 90° bend, BA = 1.57 × (R + K × T).

MaterialR/T below 1R/T 1 to 3R/T above 3
Aluminum0.330.400.50
Mild steel0.38 to 0.420.42 to 0.460.50
Stainless (verify with a test bend)0.40 to 0.440.44 to 0.480.50

Copper by hardness, from the same source: soft 0.35; semi-hard copper or brass 0.41; hard 0.45.

Machinery's Handbook's 90° bend allowance formula implies K ≈ 0.45, in line with mild steel at R/T 1 to 3.

This calculator also has its own page.

More calculators in the Toolbox

What the drawing must say

Datums from the seating flat. Datum A is the flat that seats on the mating part, usually the largest flat with the mounting holes. Datums B and C are holes, or a hole and a slot, in the same flat as A. They are cut in the same setup as A, so they are accurate, and they can be referenced at MMB when pins or clearance fasteners go through them. A cut edge is acceptable as B or C; a formed edge is a poor datum because it carries the bend error. When a channel seats on two flanges at once, make both flanges one datum rather than picking one.

Tolerance by where the feature is. Holes in the datum flat get a tight position, because they are cut together. Features on other flanges get a looser position or profile that adds the bend error for each bend in the chain. Formed flanges get a profile to A, B and C, which avoids stacking ± dimensions across bends.

A size-banded title block, not profile all over. Fabrication shops quote from a ± table with an angular tolerance, so that is the default. Use GD&T on hole patterns, key flanges and mating faces.

Dimension the formed part the way it's measured. Dimension to the outside surfaces, or to a virtual sharp (the point where the extended flat surfaces meet). Dimension each feature from its own flange. Bends drawn at 90° are 90° within the title block's angular tolerance. Don't give the outside dimension, the inside dimension and the thickness all together: that is a closed loop, and the three can't all be held.

Notes a sheet metal drawing needs:

Flat pattern. If you show one, put it on its own sheet and title it FLAT PATTERN – REFERENCE ONLY. The formed views govern.

Standards. ASME Y14.5-2018 for dimensioning and tolerancing; the material specification (for example ASTM B209 for aluminum sheet, ASTM A1011 or A653 for steel); the hardware manufacturer's installation document.

Typical tolerances

Sheet metal tolerances depend on where the feature is, not just on how tight you ask.

WhereTypical valueCost
In one flat (laser or punch)±0.13 mm for thickness under 3.3 mm; ±0.38 for 3.3 mm and up. Position in the datum flat about Ø0.25 at MMC. Hardware holes: the hardware maker's catalog size.Standard. Cut in one setup.
Across one or two bendsabout ±0.25 to 0.38 mm (±0.5 to 0.64 for thickness 3.3 mm and up); position about Ø0.76 at MMCStandard press-brake work. Tighter means fixtured forming and checking each part.
Across three or more bends±0.76 mm (±1.0 for thick sheet); position about Ø1.5 at MMCStandard. Tighter is a cost driver and often not repeatable.
Bend angle±1°Standard. About ±0.5° is possible on a well-set press brake, with in-process checks.
Tighter than these on a formed featureMachining or punching after formingAdds an operation and a fixture.

Self-clinching hardware locations follow their holes; size the holes and edge distances from the hardware maker's catalog.

Worked example: the L bracket

The L bracket from the Rapid Datum demo is 2 mm 5052-H32 aluminum, 60 × 50 mm with a 40 mm flange, and one 90° bend.

The L bracket drawing: a side view of the bent bracket with a flatness frame on datum A and a 40 dimension, a top view with datum B, a perpendicularity frame, a profile frame on the flange, and the 50 and 60 dimensions, with notes and a title block.
The L bracket drawing from the Rapid Datum demo. Open the image for the full size.
On the drawingWhat it saysWhy
Datum A, flatness 0.3 on the outer face of the long legThe leg that seats is the primary datumIt's the flat that mounts. Flatness 0.3 is realistic for a 60 mm sheet flat; tighter would need flattening.
Datum B, perpendicularity 0.2 to A, on a cut edgeThe part has no holes, so a cut edge stops it slidingA cut edge is accurate because it's cut with A's flat. A formed edge would carry the bend error.
The flange: profile 0.76 to A and BThe bent leg is within a 0.76 zone of its true positionA 0.76 zone is ±0.38, the across-one-bend value. It covers the bend angle, the radius and the flange length in one control, and nothing stacks.
60 basic, 40 ±0.4, 50The outside dimensions, measured to the outer facesOutside faces are what you measure. The 60 is basic because the flange's profile tolerance governs it.
UNLESS OTHERWISE SPECIFIED, INSIDE BEND RADII R2 ±0.5.One radius, 1× the thicknessA standard tool radius for 2 mm 5052-H32.
DIMENSIONS APPLY AFTER FORMING.The formed part is inspected, not the blankThe blank size is the shop's job, from its own K-factor.
Thickness only in the material callout (2 THK)No separate inside dimensionsGiving 40, 38 and 2 together would form a closed loop.

A bracket with mounting holes would use a hole in the seating flat as B and a second hole or slot as C, both at MMB, with the flange still profiled to A, B and C.

Common mistakes

  1. Holes too close to a bend. They stretch into ovals and move. Keep holes about 4T or more from the bend, or add them after forming.
  2. No bend relief. Where a bend runs out at an edge, the corner tears or bulges. Add a relief cut at least T wide and at least as deep as the bend radius.
  3. Machining tolerances on formed features. ±0.05 across a bend can't be held by bending alone. Use the across-bend values, or plan a machining step after forming.
  4. Thickness by gauge alone. "14 GA" is 1.9 mm in steel and 1.6 mm in aluminum. Write the thickness, and put the gauge in parentheses if you want it.
  5. Dimensions that close a loop or chain across bends. Giving the outside dimension, the inside dimension and the thickness all together, or chaining from one edge over several bends, gives the shop impossible or stacked requirements. Dimension each feature once, from its own flange or the datums.

Questions

What is the minimum bend radius for sheet metal?

It depends on the alloy, the temper and the thickness. A common default is an inside radius equal to the thickness. Harder tempers need more, and going below the alloy's minimum cracks the outside of the bend. Use one radius for the whole part so the shop needs one tool.

What is a K-factor?

The position of the neutral line inside the bend, as a fraction of the thickness from the inside surface. It is typically 0.3 to 0.5, rising with the bend radius. It sets the bend allowance, and so the flat blank size. The shop chooses it for its own tooling, which is why the drawing gives formed dimensions.

How close can a hole be to a bend?

Keep holes about four times the material thickness or more from a bend. Closer holes stretch when the flange is formed. If a hole has to be closer, add it after forming.

What tolerance can sheet metal hold?

About ±0.13 mm for features cut in one flat of thin sheet, about ±0.25 to 0.38 mm across one or two bends and ±0.76 mm across three or more, with ±1° on bend angles. Tighter values on formed features need machining or fixtured forming.

Should a sheet metal drawing include a flat pattern?

Only as a reference. The formed views govern, and the shop develops its own flat from its K-factor and tooling. If you include one, title it "flat pattern, reference only".

Sources

More guides