Designing and drawing castings and forgings
A casting drawn like a machined part causes trouble in both directions. The foundry has no definition of the raw part, so it guesses at draft, radii and stock. The machine shop has no reliable place to pick the part up, so the first cut takes too much off one side and leaves black spots on the other. ASME Y14.8 fixes this with two linked drawings and datum targets. This guide covers the design rules for cast and forged parts, what each drawing must say, and the tolerances each process holds.
Design rules for castings and forgings
A casting is poured or injected into a mold, and a forging is squeezed into a die. Either way, the part has to fill, cool or flow evenly, come out of the tooling, and leave enough material where it will be machined.
| Rule | Typical value | Why |
|---|---|---|
| Even sections, gradual transitions | avoid isolated heavy sections; keep section changes under about 2:1 and blend them with a taper of about 1:4 | Heavy spots cool last and shrink, leaving porosity or sink. In forgings they fill last and need more force. |
| Draft | sand castings about 2° (1° at the least); die castings a minimum of about 0.3° (zinc) to 0.7° (brass) by alloy; forgings at least about 3° on aluminum and 5° to 7° on steel. More on inside walls and deep pockets | The part has to release from the mold or die. Inside walls grip as the metal shrinks onto the core or die. |
| Fillets and radii everywhere | no sharp inside corners; on forgings at least about 3 mm, rising to about 6 mm on ribs over 75 mm tall | Sharp corners cause hot tears in castings, poor die fill and laps in forgings, and stress risers in service. |
| Minimum wall | sand casting about 2.5 to 3 mm in aluminum, 3.3 to 6 mm in steel; die casting about 0.6 mm (zinc) to 1.3 mm (magnesium, brass); investment casting about 1.5 mm, less in small areas | Thinner walls don't fill reliably. |
| Machining stock | per surface, for parts about 100 to 250 mm: sand casting about 1.5 to 4 mm (more on the cope face and on large or hand-molded castings); investment about 0.4 to 1.8 mm; die casting about 0.25 to 1.5 mm. Forgings: at least about 1.6 mm up to 200 mm, rising to about 4.8 mm over 900 mm | The first cut has to get under the cast or forged skin and absorb the tolerance, draft and mismatch, but not go so deep that it exposes porosity. A bore machined all round carries the stock on each side. |
| Parting line | flat if possible, with no undercuts in either half, placed so critical features sit in one half | Features in different halves pick up mismatch between the halves. |
| Supplier input | agree the parting line and process with the foundry or forge before the design is final | They know where gates, risers and flash go, and what the tooling can do. |
More calculators in the Toolbox
What the drawing must say
Standard. ASME Y14.8-2022 covers castings, forgings and molded parts, together with Y14.5-2018. State it in a note, for example CASTING REQUIREMENTS IN ACCORDANCE WITH ASME Y14.8-2022.
Two drawings, not one with a machining allowance. Y14.8 recommends separate drawings: an as-cast (or as-forged) drawing that fully defines the raw part, and a machining drawing that calls up the casting by part number and revision and defines the finished part. The older practice of drawing only the finished part with a machining-allowance note was removed in the 2022 edition, because it leaves the raw part undefined. The as-cast drawing and model must carry every parting line, draft angle, radius and the machining stock.
As-cast datums are datum targets. On a prismatic part, usually a 3-2-1 pattern: three targets for A, two for B, one for C, each at a basic location. Round parts use other patterns, such as target lines or equalizing pairs. Place them:
- all of one datum's targets in one mold or die half, so mismatch can't tilt the frame;
- on surfaces that stay as cast, opposite the first machining cuts, so the stock comes off evenly;
- away from parting lines, flash, gates, risers and ejector pads.
More calculators in the Toolbox
Machined datums come from the as-cast ones. The machining drawing continues the lettering. D is the first machined face, located by profile to A, B, C. E is a machined bore, positioned to A, B, C and perpendicular to D. F is a clocking feature. Every other machined feature then refers to D, E, F. Y14.8 requires the drawing to state this relationship between the two frames.
Notes an as-cast drawing needs:
- The Y14.8 note, and that untoleranced dimensions are basic with a general profile to the datum targets.
- Draft: defined in the model or by an angle, and how dimensions relate to it.
- Radii: the fillet and corner radii, and the maximum radius on corners drawn sharp.
- Wall thickness, where a uniform wall must be held.
- Parting line, shown with its symbol, with the maximum mismatch and flash.
- Gates, risers and other remnants: whether they're within the tolerances or how far they may stand proud.
- Whether machining of as-cast surfaces is permitted, and if so the texture required.
- Material with its casting designation and temper, for example
A356.0-T6 ALUMINUM SAND CASTING PER ASTM B26, plus heat treatment and hardness checks. - NDE with acceptance criteria, always stated, even if it's "visual only".
- Marking: part number, foundry mark and heat code, with their location.
Forgings add: the forging plane (draft is measured from it); the parting line symbol, which is mandatory on closed-die forgings; flash, trim and mismatch limits; grain direction where it matters, shown with an arrow or by a note that the grain flow follows the part outline; and test locations.
Typical tolerances
Casting tolerances depend mainly on the process and the size of the part. These are typical values at about 100 mm. ISO 8062-3 grades castings (CT or DCTG grades), NADCA publishes die-casting tables, and forgers work to the Forging Industry Association guidelines or EN 10243-1. Agree the grade with your supplier.
| Process | As-cast tolerance at about 100 mm | As a general profile | Cost and notes |
|---|---|---|---|
| Sand casting | about ±1.5 to ±3 mm (roughly CT10 to CT12); machine-molded and shell about ±0.8 to ±1.6 | about 3 to 6 mm to the datum targets | Cheapest tooling, loosest part. Machine anything that mates. |
| Investment casting | about ±0.3 to ±0.5 mm (roughly CT5 to CT7); tighter by arrangement | about 0.6 to 1.1 mm | Costlier per part; less machining. |
| Die casting | aluminum, within one die half: about ±0.33 mm standard, ±0.13 mm precision (NADCA); more across the parting line | about 0.6 mm | Expensive tooling, cheap parts at volume. |
| Closed-die forging | about ±0.8 mm (FIA guideline: ±0.003 mm per mm, ±0.8 minimum), plus die wear, die closure (about +1 mm and up across the parting line) and mismatch (about 0.5 mm and up) | — | Each allowance is stated separately. Forgers can often hold tighter by agreement. |
| Machined features | machining capability (see the CNC guide) | — | To the machined datums D, E, F. |
Dimensions across the parting line also carry die closure and mismatch. Keep critical relationships within one half of the mold, or budget for both.
Worked example: an aluminum housing (illustrative)
An A356.0-T6 sand-cast housing, about 150 mm long, has a machined mounting face and a machined bearing bore. The diagram is an illustration, not a drawing from the app.
| Drawing | On the drawing | Why |
|---|---|---|
| As-cast | Datum targets A1, A2, A3 on the back face; B1 and B2 on a side; C1 on an end; all in the cope (top half), at basic locations | The fixture touches six defined points that stay as cast. |
| As-cast | General profile 5 mm to A, B, C, untoleranced dimensions basic | One control for the whole as-cast shape, at what sand casting holds. |
| As-cast | Draft 2° outside, 3° inside; fillets R3 unless otherwise specified; parting line with its symbol; mismatch and flash limits; 2 mm machining stock in the model on the mounting face and bore | The raw part is fully defined, so the foundry and the machine shop can each be held to it. |
| As-cast | Material, heat treatment and hardness note; radiography with a named acceptance class on the bore wall | Porosity in the bearing area would show up only after machining. |
| Machining | MACHINE FROM CASTING PN ... REV ...; the targets repeated with the same labels and basic locations | The machine shop fixtures the casting exactly as the foundry inspected it. |
| Machining | D: mounting face, profile to A, B, C plus flatness. E: bore Ø42 H7, position to A, B, C, perpendicular to D. Mounting holes to D, E, F | The machined frame is tied to the cast frame, so the stock comes off evenly and the finished features relate to each other. |
Common mistakes
- A finished-part drawing with a machining allowance note. The raw casting is then undefined: no draft, radii, parting line or stock that anyone can be held to. Y14.8-2022 removed that method. Make an as-cast drawing and a machining drawing.
- Datums on surfaces that get machined away, or targets split across both mold halves. The frame disappears after machining, or mismatch tilts it.
- Machining tolerances on as-cast surfaces. A sand casting can't hold ±0.1. Use a general profile at what the process holds, and machine the features that mate.
- Draft left to the foundry and not defined. The tool maker adds it anyway, and nobody can tell where the dimensions apply on a drafted wall. Put draft in the model or on the drawing.
- No inspection or acceptance stated. "Sound casting" isn't a requirement. Name the NDE method and acceptance class, or say that visual inspection only is required.
Questions
What is the difference between an as-cast drawing and a machining drawing?
The as-cast drawing defines the raw casting: its shape, draft, radii, machining stock, parting line and datum targets. The machining drawing calls up that casting by part number and defines the finished part, with machined datums tied back to the as-cast ones. ASME Y14.8 recommends keeping them separate.
What are datum targets on a casting?
Specific points, lines or small areas on the raw surface that the part rests on for setup and inspection. On a prismatic part that is usually three for datum A, two for B and one for C. Rough cast surfaces are too irregular to contact as a whole, so targets give a repeatable pickup.
How much machining allowance does a casting need?
For a part about 100 to 250 mm long, typically about 1.5 to 4 mm per surface on sand castings, 0.4 to 1.8 mm on investment castings and 0.25 to 1.5 mm on die castings. Large and hand-molded castings need more. The first cut has to get under the cast skin and cover the casting tolerance, without cutting so deep that it exposes porosity. Agree the value with the foundry; ISO 8062-3 calls it the required machining allowance.
What draft angle does a casting need?
Sand castings typically take about 2°, and 1° at the least. Die castings need much less, a minimum of about 0.3° to 0.7° depending on the alloy. Inside walls and deep pockets need more, because the metal shrinks onto them. Forgings need at least about 3° on aluminum and 5° to 7° on steel.
Which standard covers casting and forging drawings?
ASME Y14.8-2022, together with ASME Y14.5-2018 for dimensioning and tolerancing. The 2022 edition removed the old practice of drawing only the finished part with a machining-allowance note.
Sources
- ASME Y14.8-2022, Castings, Forgings, and Molded Parts, and ASME Y14.5-2018, Dimensioning and Tolerancing
- Engineers Edge, Sand casting design (sand draft, minimum walls, section changes)
- Engineers Edge, Forging design (forging draft, fillets, parting line)
- Wikipedia, Die casting (minimum draft and section by alloy)
- Wikipedia, Forging (forging draft)
- Kurt Foundry, What is machining allowance in casting (machining stock by process and size)
- Manufacturing Network, Sand casting guide (minimum walls, stock, tolerances)
- FacFox, ISO 8062 casting tolerance grades by process (CT grades; a secondary reproduction of ISO 8062)
- Ruger Investment Casting, Tolerances (Investment Casting Institute normal and premium tolerances)
- Engineers Edge, Casting tolerances per NADCA and ISO (die-casting tolerances)
- Forging Industry Association, Product Design Guide for Forging (Appendix A: forging tolerances, finish allowance, draft)
- ISO 8062-3, Geometrical product specifications: dimensional and geometrical tolerances for moulded parts, Part 3: castings