Designing and drawing die castings
A die cast part is made by forcing molten metal into a steel die under high pressure. The die opens along a parting line, and the part has to come out of it. Most die casting drawing problems come from forgetting that the die has two halves and moving cores.
Two processes
- High-pressure die casting (HPDC) fills the die fast, at roughly 700 to 2,500 bar. It gives quick cycles and the thinnest walls, and it is used for aluminium, zinc and some magnesium. It has the highest porosity risk.
- Low-pressure die casting (LPDC) fills slowly, at roughly 0.7 to 1.5 bar. It suits complex shapes, larger parts and lower-melting alloys, with less porosity. It struggles with walls under about 3 mm.
Both are for nonferrous alloys. Name the process on the drawing, because the wall and draft rules differ.
Design rules
Walls
- Typical wall ranges: HPDC 2 to 4 mm (0.08 to 0.16 in); LPDC 3 to 5 mm (0.12 to 0.20 in). Confirm the minimum and maximum with the caster for your alloy.
- Keep walls uniform, ideally within ±10% of nominal. Uniform walls cool evenly and hold tolerance better.
- Blend thick sections into thinner ones with radii, not sharp steps.
Ribs
- Make ribs 70 to 80% of the nominal wall thickness, so they do not sink or stress the casting.
- Add ribs to a boss when its height is more than its diameter.
Bosses
- Keep bosses short. Keep at least 6.5 mm (0.25 in) between adjacent bosses to limit porosity.
- Keep wall thickness uniform around each boss, fillet its base, and give it draft.
Draft
- Put draft on every face that is parallel to the die opening direction, so the part can eject without scraping.
- One to two degrees is generally enough, and it matters most on faces aligned with the die opening. Internal geometry that works with ejectors is typically 3 to 5 degrees. [Fictiv, p.22 and p.26]
- Put the standard draft in a general note (for example "UNLESS OTHERWISE SPECIFIED, DRAFT 1° MIN"), and call out only the exceptions on the faces. Say which end the dimensions apply to, and whether the draft adds or removes material.
Fillets
- Use fillets of at least 1 mm at every junction, with a consistent radius. Sharp corners crack and fill badly.
Parting line
- The parting line is where the two die halves meet. Flash forms along it and is trimmed afterwards, so put it where it does not hurt appearance or function.
- Features across the parting line, or formed by a moving slide, need a looser tolerance than features within one die half.
- The parting-line tolerance grows with the projected area of the part, so a large part gets a looser one. [Fictiv, chart p.22] Use the direction, not the numbers.
Holes, undercuts and threads
- Cored holes need more draft than the outside faces, because the metal shrinks onto the core as it cools. Keep the wall around a hole within ±10% of its average wall thickness, and avoid sharp corners near it.
- Avoid undercuts. They need side slides, add cost, and should be shallow and aligned with the parting line.
- Cast threads need flash trimmed, so decide whether to cast the thread or cast a hole and tap it.
Ejector pins
- Plan roughly one ejector pin per 4 to 8 square inches of die surface. [Fictiv, p.26]
- Put ejector pins on non-functional or machined areas. Fictiv suggests pins at least 10 mm (0.38 in) in diameter there.
- Ejector bosses give a pin a flat landing. Boss height is a minimum of 1.5 to 2 times the ejector pin diameter. [Fictiv, p.26]
Tolerances
- State the general tolerance on the drawing, for example "ISO 8062-3 DCTG 7". DCTG 6 to 10 is one vendor's quoting default, not a rule, so do not rely on it when no tolerance is given. [Fictiv, p.48]
- ISO 8062-3:2023 Annex A gives the pressure die casting grades. For light metals, the grade grows with the largest dimension: 6 up to 50 mm, 7 from 50 to 180 mm, 8 from 180 to 500 mm, 9 above 500 mm. Zinc is 3 to 6 and copper is 6 to 8. [ISO 8062-3:2023 Annex A]
- Tighten a feature only where the function needs it. A tight tolerance on a die cast part usually means a machining operation after casting.
Mismatch and flash
Mismatch is the step where the two die halves do not line up. Flash is the thin fin of metal that squeezes out at the parting line.
- Mismatch is called out separately from the tolerance grade (ISO 8062-3 clause 6 and ISO 10135). Agree the limit with the caster, and do not put a number on the drawing until the caster has given one.
- No source we hold gives numeric limits for flash. Agree them with the caster as well.
What the drawing must say
- The die casting process (HPDC or LPDC) and the alloy.
- Where the parting line is, and which surfaces are cosmetic.
- Draft: a general draft note, the exceptions on the faces, and which end the dimensions apply to.
- Which holes are cored and which are drilled, and any drill allowance.
- The tolerance grade for the features, or the note "per DCTG [grade], agreed with the caster".
- Machining allowance on surfaces to be machined, for example an ISO 8062-3 RMAG grade.
- The first machining setup is located from the as-cast surfaces. The machined datums take over after that.
- Where ejector marks and gate and overflow remnants are acceptable, and how far they may stand proud of or sit below the surface.
Common mistakes
- No draft on a core face. The part sticks in the die.
- Parting line on a cosmetic surface. Flash shows.
- A thick boss on a thin wall. Porosity and sink.
- A tight tolerance across the parting line. Mismatch eats it.
Questions
Is die casting the same as casting?
No. Die casting forces metal into a reusable steel die under pressure. Sand and investment casting use expendable moulds that are broken away after each casting, and gravity (permanent-mould) casting pours into a reusable metal mould without pressure. The rules here are for die casting.
Do I need machining after die casting?
Often for tight holes, faces and threads. Show the machined surfaces on the drawing with their own datums.
How much draft does a die casting need?
One to two degrees is generally enough, and it matters most on faces aligned with the die opening. Internal geometry that works with ejectors is typically 3 to 5 degrees. Put the standard draft in a general note and call out only the exceptions.